Curing chambers: temperature, humidity and where rejects come from
In the curing chamber the green sheet gains the strength to be taken off the pallet without breaking. Three things cause rejects here: heat applied before the cement began to set; temperature raised too fast or unevenly; the sheet losing water to dry air and drafts.
In short
7minutes to read
7sections
5sources
3catalog items
In this article
- 01What the owner and the buyer need to decide
- 02What happens to the sheet in the chamber
- 03Four parts of the mode and where rejects arise in each
- 04Humidity and drafts
- 05How to link a reject to the chamber
Contents
The curing chamber is needed so that the green sheet gains, in a short time, enough strength for demolding, cutting and stacking. Cement hardens faster in warmth and humid air. But warmth and moisture help only if they are supplied at the right moment and evenly. Rejects in the chamber most often come from three mistakes. The sheet is heated before the cement has begun to set. The temperature is raised too fast or unevenly across the volume of the chamber. The sheet dries out: the air is dry, there are drafts, the door stands open. The chamber mode (time, temperature, humidity) is set by the process regulations of your line. This article covers what it depends on and what to check when rejects appear.
What the owner and the buyer need to decide
The chamber is not a machine with spare parts but a warm, humid room with steam, ventilation, sensors and doors. Money is lost on rejects in it not because of wear but because the mode is not held. So the first things needed are:
- Records. Temperature and humidity sensors at several points of the chamber and a time record. Without a record, the argument "is the chamber at fault or the mix" cannot be settled;
- Uninterrupted steam. If the boiler or the steam line does not supply steam evenly, the chamber drifts out of mode. This is a matter for the boiler house and the steam line;
- Doors and seals. Gaps and open doors give drafts and dry, cold air at the outer stacks;
- Demolding by strength, not by the clock. If the sheet is taken off before it has gained strength, the demolding machine breaks it and delaminates it at the edge.
What happens to the sheet in the chamber
The green sheet after the forming machine is a wet mass of cement and fibre laid on a pallet or template. The cement reacts with water and gradually turns into stone. Heat speeds up the reaction, and the reaction needs water all the time: if the sheet dries out, hardening stops and the strength is not reached.
The textbook literature on asbestos cement describes this scheme. The sheets harden in steam curing chambers at elevated temperature and high humidity. Then they are held in a heated finished-goods store until they gain the strength for shipment. If the plant has an autoclave and the cement is mixed with sand, hardening takes place in the autoclave under steam pressure, and the hold in the store is not needed.
Air-cured fibre cement also has a pre-curing step before the store. Patents on fibre cement describe it like this: after forming and the press, the sheet is held on the pallet, if desired in conditions that keep the temperature, the humidity or both. The sheet then warms itself from the heat of the cement reaction. After that the sheets are restacked and left to harden in air for several weeks. The mode depends on the mix composition, the type of product and the line; there is no single recipe.
Four parts of the mode and where rejects arise in each
For the heat treatment of cement products, the mode is usually divided into four parts. This is how it is described by both precast concrete builders and textbooks on heat and moisture treatment.
| Part of the mode | What it is for | What goes wrong |
|---|---|---|
| Hold before heating | the cement begins to set at normal temperature | heat applied at once: internal stresses, a network of cracks, a weak sheet |
| Temperature rise | heat the sheet evenly | too fast: a temperature difference across the thickness and across the stack, cracks |
| Hold at temperature | gaining strength | hot and cold zones in the chamber: sheets of different strength in one stack |
| Cooling | prepare the sheet for exit | a sharp difference with the shop or the outdoors, especially in winter: cracks, warping |
A stepped or smooth temperature rise is chosen precisely to reduce the temperature difference across the section of the product. For concrete, sources directly link heating that is too fast before setting begins with thermal shock and cracks. Too high a holding temperature is also harmful for concrete: a product that later serves in a humid environment may crack years afterwards. The limit values are set by standards and regulations; figures from concrete cannot be transferred directly to slate.
Humidity and drafts
The sheet in the chamber should not dry but harden. When the air is dry, water leaves the surface and edges faster than it arrives from inside. The surface and the edge shrink, the middle does not, and cracks run along the edge.
This mechanism is well described in a study of air-cured fibre cement sheets. Edge cracks appeared in the stacks while the sheets were still drying in the pile. The cause was that water left the side of the stack faster than the moisture evened out inside the stack. Most cracks were on the sunny side of the stacks and in dry months. In the chamber the same is caused by a draft at the door, outer stacks by a cold wall, and a dry spot next to a fan.
What to check:
- air humidity at different points, not by one sensor at the entrance;
- where cold air comes into the chamber from: doors, gates, gaps, exhaust;
- whether drops of condensate fall from the ceiling onto the sheets: wet spots give different color and different strength;
- whether the stacks are covered, if the chamber does not hold humidity by itself.
How to link a reject to the chamber
| What you see | Where to look |
|---|---|
| A network of fine cracks over the whole surface | early or too fast heating |
| Cracks along the edge at the outer stacks | dry air, a draft, a cold wall |
| Different strength of sheets in one stack | uneven temperature across the chamber |
| Sheets break at demolding | not enough strength: too little time or over-drying |
| Spots and different color | condensate dripping onto the sheets |
| Warping of a flat sheet | different humidity on the top and bottom of the sheet |
This is a scheme for searching. The same reject can come from the mix or the press; the chamber is checked together with them.
What the process engineer should do
- Compare the actual temperature and humidity record with the regulations for the shifts with rejects.
- Mark which place in the chamber and which row of the stack the rejects come from.
- Check whether the hold time before steam is applied is kept when the chamber is overloaded.
- Check the steam supply: the pressure at the chamber inlet, the work of the steam traps, and whether water rather than steam is going into the chamber.
- Before demolding, check the strength of control samples, if the regulations provide for it.
How we do it
- From the photo, dimensions and the passport of the unit, we look for the item at the manufacturing plant. What we find, with the price, photos and specifications, we send before the order.
- We inspect the lot at the plant before shipment: part number, dimensions, lot, packaging.
What this article relies on
Below are the documents and materials we refer to, so that you can check what is said for yourself.
Reference materials
- Rybyev I. A. "Building Materials Science" (Строительное материаловедение), section "Fundamentals of asbestos-cement product manufacturing": hardening in steam chambers at elevated humidity, the hold in a heated store, the autoclave with sandy cementstudme.org ↗
- Fiorelli J. et al. "Durability of fibre-cement roofing corrugated sheets", XIII CIB Conference on Durability of Building Materials (CIB DC33112): edge cracks in stacks from uneven water loss, the link with dry periodsirbnet.de ↗
- CPCI Technical Bulletin "Curing of High Performance Precast Concrete": hold before heating, controlled temperature rise, thermal shock, limit of the holding temperaturesaraschok.com ↗
- Stages of heat and moisture treatment and stepped temperature rise to reduce the difference across the section — Belarusian National Technical University, repositoryrep.bntu.by ↗
- Patent US 11773023 "Methods for producing air-cured fiber cement products": pre-curing of the sheet in controlled conditions, heating from the cement reaction, further hardening in airpatents.google.com ↗
The four parts of the mode and the table "reject: where to look" are drawn up from the general rules of heat treatment of cement products; the mode of your chamber follows the process regulations.