Slate is checked for bending strength and strength under load, for density, impact toughness, water tightness, water absorption and frost resistance. The methods for corrugated sheets are now in GOST 30340-2012, for flat sheets in GOST 18124-2012; before that they were in GOST 8747-88. Each test answers its own question about the sheet, and each has its own specimen preparation.
In short
5minutes to read
4sections
3sources
4catalog items
In this article
Slate is tested to confirm that the lot carries its load, is dense enough, does not fear impact, does not let water through and survives winters. For a corrugated sheet the methods are now collected in GOST 30340-2012, for a flat one in GOST 18124-2012. In 2013 both standards replaced GOST 8747-88 in this respect, but many laboratories still work by it. There are seven tests: bending, load on a whole sheet, density, impact toughness, water tightness, water absorption and frost resistance. Some are done on every lot, some periodically. Below is what each one shows and how it is set up.
What the owner and the process engineer need to decide
- Which tests to do in house. Acceptance tests (appearance, dimensions, load, density) go on every lot. It is more convenient to do them in your own laboratory. The periodic ones for a corrugated sheet are bending and impact toughness at least once a month, and frost resistance and water tightness at least once a quarter. For a flat sheet, bending is part of the acceptance of every lot, and impact toughness and frost resistance are checked periodically. The periodic tests can be given to an outside laboratory if you have no chamber of your own.
- Which document the laboratory works by. If the logs and reports cite GOST 8747-88 while the quality document cites GOST 30340-2012, the buyer has the right to ask a question. It is better to bring the methods in line with the current standards.
- What to do with the result. A test is not just a mark for a document. A drop in strength or density is the first sign that something on the line has shifted: the mass, the felt, the press or curing.
The tests one by one
Bending strength
What it shows. How strong the sheet is as a material.
How it is done. A specimen is cut from the sheet, placed on two supports and loaded at mid-span until it breaks. The load is raised smoothly, at a set rate. The ultimate strength is calculated from the breaking load, the span and the dimensions of the cross-section. A corrugated sheet can also be tested whole, in which case the section modulus of the profile is used in the calculation. Before the test the specimens are conditioned indoors so that they are air-dry.
Load on a whole sheet
What it shows. Whether the sheet will withstand what will be on the roof: snow, a person during installation.
How it is done. The sheet is placed on supports and the specified load is applied through a bar across the width of the sheet or through a wooden punch at one point. The sheet must carry it without failure. This is a pass/fail check, not a measurement.
Density
What it shows. How tightly the mass is packed. Density is directly related to strength and water absorption.
How it is done. Specimens are dried in a drying oven at 105–110 °C for at least 24 hours and weighed. Then they are saturated with water and weighed in air and in water. The difference in mass gives the volume of the specimen and the density.
Impact toughness
What it shows. How the sheet takes impact: hail, a dropped tool, careless unloading.
How it is done. Narrow specimens are saturated with water and broken with a pendulum impact tester. The work spent on breaking is divided by the cross-sectional area of the specimen.
Water tightness
What it shows. Whether the sheet lets water straight through.
How it is done. Water is poured into a wave trough of a corrugated sheet, or into a frame on the surface, and left for a day. Then the underside is examined. Drops there mean the sheet has failed.
Water absorption
What it shows. How much water the sheet takes up. High water absorption is a path to cracking in frost.
How it is done. The mass of a dry specimen is compared with that of a specimen saturated with water. In the new standards this is a recommended method in an annex, not a mandatory requirement.
Frost resistance
What it shows. Whether the sheet will survive many winters.
How it is done. A pair of specimens is cut from each sheet: one main, one control. The main ones are saturated with water and repeatedly frozen in a chamber and thawed in water. Then they are inspected (there must be no delamination) and broken in bending together with the controls. The sheet has passed if, after the cycles, it keeps the required share of its strength. The number of cycles and the threshold are set by the standard.
Where mistakes are most often made
- Specimens are not taken from different stacks, or the outer sheets of a stack are taken. The standard requires taking sheets from different stacks, without picking the best and the worst.
- Specimens are not conditioned before the test. A wet specimen gives a different bending result than an air-dry one.
- The load is applied with a jerk. The loading rate is set, and it must not be exceeded.
- Specimens are not marked. Later it cannot be proved which lot the sheet came from.
- The log is kept on scrap paper. Test logs are an official document of the manufacturer.
How we do it
- From the photo, dimensions and the passport of the unit, we look for the item at the manufacturing plant. What we find, with the price, photos and specifications, we send before the order.
- We inspect the lot at the plant before shipment: part number, dimensions, lot, packaging.
What this article relies on
Below are the documents and materials we refer to, so that you can check what is said for yourself.
Standards and documents
- GOST 30340-2012 "Chrysotile-cement corrugated sheets. Specifications", the section on control methods and annexes A, B; what it replacestext ↗
- GOST 18124-2012 "Chrysotile-cement flat sheets. Specifications", the section on methods and the annexes on water tightness and water absorptiontext ↗
- GOST 8747-88 "Asbestos-cement sheet products. Test methods": the set of methods and the status of partial replacement (prg.kz)text ↗
Test conditions (loading rate, temperatures, soak times, number of cycles) are in the text of the standard; this is a retelling of the principle without figures.