0In the list
02Defects and testing

Sheet thickness varies across or along: what has gone wrong

Thickness that varies across the width of the sheet almost always comes from an uneven layer building up on the screen or felt: a clogged screen, a skewed or worn felt, uneven vacuum across the width. Thickness that varies along the length and from sheet to sheet comes from slurry concentration and the number of turns on the format drum.

Updated 5 min read

In short

5minutes to read

7sections

7sources

4catalog items

In this article

  1. 01What the standard allows
  2. 02How the thickness builds up
  3. 03Thickness varies across the width
  4. 04Thickness wanders along the length and from sheet to sheet
  5. 05How to look for the cause
Contents
  1. What the standard allows
  2. How the thickness builds up
  3. Thickness varies across the width
  4. Thickness wanders along the length and from sheet to sheet
  5. How to look for the cause
  6. What to order afterwards
  7. How we do it

The thickness of a sheet is the sum of the thin layers picked up by the cylinder screens and wound on by the format drum. If the sheet is thicker at one edge, the layer across the width of the machine is building up unevenly. The suspects are the screen, the felt and the vacuum boxes. If the thickness wanders along the length or from sheet to sheet, look at the slurry concentration, at the feed into the vats and at how many turns the drum manages to wind. First measure the thickness to a pattern, then decide which unit to replace.

What the standard allows

GOST 30340-2012 sets for corrugated sheets a nominal thickness and limit deviations from it. The tolerance depends on the profile and thickness, usually fractions of a millimetre in each direction. Flat sheets have their own tolerances in GOST 18124-2012, and for thick sheets they are wider. The European standard for profiled sheets, EN 494, also sets a thickness tolerance. Manufacturers state it in the declarations for their sheets.

Note that under GOST the thickness of a sheet is taken as the average of four measurements, one in the middle of each side. So a sheet can pass on the average and still be noticeably thinner at one edge. Formally this is not a thickness defect, but the buyer will see the difference, and a thin edge is a weak spot of the sheet.

How the thickness builds up

Each vat with a cylinder screen gives the felt a thin film. The felt passes through all the vats in turn, collects several films and carries them over the vacuum boxes. The format drum winds this layer on turn after turn. When the thickness on the drum reaches the required value, the blank is cut off.

From this you can see where a difference may arise:

  • across the width, if the screen, felt or vacuum do not work equally across the width;
  • along the length and from sheet to sheet, if the thickness of the film changes with time: the slurry concentration floats, the level in the vat, the felt speed;
  • at the joint of the blank, where winding starts and ends.

On modern lines an electronic thickness gauge measures the blank, and the control system adjusts the slurry and water feed by itself. But automation evens out the average thickness. It will not correct a skew across the width.

Thickness varies across the width

Cylinder screen

A screen clogged over part of its width picks up a thin layer there. A torn or dented screen gives a stripe. The check is to inspect and wash the screen. If the stripe stays in one place on the sheet and matches a place on the screen, the cause is found.

Felt

The felt works differently across the width when:

  • it clogged unevenly, for example the edges are washed worse than the middle;
  • it stretched and runs off, lying with a skew or a fold;
  • the tension at the edges differs;
  • the batt has worn through over part of the width.

A patent on felts for fibre cement describes a pressure roll at each cylinder screen. It regulates how much slurry the cylinder gives to the felt. If the pressure across the width is unequal, the layer will be unequal too.

Vacuum boxes

The box draws water out through the felt. A worn cover, an air leak at one edge or clogged holes give different moisture in the layer across the width. A wet area after pressing is compacted differently from a dry one, and the thickness diverges.

Format drum and pressure rolls

If the drum runs out of true, if a layer of slurry has stuck to it or the coating is worn, the layers lie unevenly. Uneven pressure of the rolls across the width has the same effect. A patent on profiled format drums shows directly that the shape of the drum surface sets the thickness of the sheet across the width. So wear or build-up on the drum changes it as well.

Thickness wanders along the length and from sheet to sheet

  • Slurry concentration. If the slurry going into the vats is now thick, now thin, the film comes out now thick, now thin.
  • Level in the vats and the feed of slurry across the width of the vat.
  • Felt speed and the moment the blank is cut.
  • Calibration of the thickness gauge. If the sensor is off or dirty, the automation holds the wrong thickness.

How to look for the cause

  1. Measure the thickness on several sheets at the same points: at both edges, in the middle, at the start and the end of the sheet.
  2. Plot the measurements on a diagram. A stripe in one place means the screen or felt. One edge thinner along the whole length means the felt, tension or vacuum on that side. A difference from sheet to sheet means slurry and feed.
  3. Check whether the stripe matches a place on the screen or felt. For this it helps to mark the edge of the felt.
  4. Check the vacuum readings by box and the records of slurry concentration.
  5. Only after that decide whether to replace the felt or the screen.

What to order afterwards

  • Felt. If it is stretched or clogged and washing does not help. To order you need the slurry, type of fabric, density and size from the machine's passport.
  • Screen, with the cylinder dimensions and the mesh number.
  • Parts for the vacuum boxes: covers and seals, to a drawing or a sample.

How we do it

  • From the tag, photo and dimensions of the old felt, we look for the item at the manufacturer. What we find, with the price, photos and specifications, we send before the order.
  • We inspect the lot at the plant before shipment: part number, dimensions, lot, packaging.

What this article relies on

Below are the documents and materials we refer to, so that you can check what is said for yourself.

Standards and documents

  • GOST 30340-2012 "Chrysotile-cement corrugated sheets. Specifications": nominal thickness and limit deviationstext ↗
  • GOST 18124-2012 "Chrysotile-cement flat sheets. Specifications": thickness deviations of flat sheetstext ↗
  • Declaration of performance of profiled fibre-cement sheets to EN 494 (Eternit Baltic): thickness tolerancetext ↗

Reference materials

  • Rybyev I. A. "Building Materials Science" (Строительное материаловедение), section "Fundamentals of asbestos-cement product manufacturing": building up the layer on cylinder screens and the format drumstudme.org ↗
  • Patent US 9415564 "Felt for forming fiber cement articles": pressure roll at the cylinder screen, film thicknesspatents.google.com ↗
  • Patent US 10144150 "Hatschek process for the production of fiber cement plates": shape of the format drum surface and sheet thickness across the widthpatents.google.com ↗
  • taminota.com catalog: TMN-XHB-09, an electronic thickness gauge with automatic adjustment of the slurry feed.

The search scheme based on measurements is drawn up from the design of the Hatschek machine, without a separate external source.

Related catalog items

  • 001

    Asbestos-cement forming felt 94047 · 1700 g/m²

    TMN-XHB-F01Xinhuibo

  • 002

    Fiber-cement forming felt 94047-1 · 1650 g/m²

    TMN-XHB-F02Xinhuibo

  • 003

    Needle-punched forming felt 51291 · 1000 g/m²

    TMN-XHB-F03Xinhuibo

  • 004

    Synthetic fiber forming felt 97049 · 1800 g/m²

    TMN-XHB-F04Xinhuibo

For slate plants

Felts, meshes and units for your line

We select from manufacturing plants in China by nameplate photo and machine dimensions. Send a photo of the plate and we will tell you what can be ordered.

Request

Ask about your machine

A part number is enough. A drawing or a photo of the unit speeds up sourcing but is not required.