Painting slate: which paint and at what stage
At the plant, slate is painted in two ways: on the fresh, not yet hardened sheet, or on the hardened one. A fresh sheet is painted so that the paint also blocks the path of efflorescence, which comes out just as the cement hardens. A hardened sheet is simpler to paint in terms of process, but efflorescence and dust must be removed before painting. Most often acrylic water-based dispersions designed for a cement substrate are used; silicate compositions less often. Colour, evenness and abrasion resistance of the coating are checked to GOST.
In short
5minutes to read
6sections
8sources
2catalog items
In this article
- 01What the owner and the process engineer need to decide
- 02Fresh sheet or hardened
- 03Which paints
- 04Where painting defects come from
- 05What is checked to GOST
Contents
Coloured slate is obtained in two ways: it is coloured in the mass (pigment is added to the slurry) or a coating is applied to the surface. The coating is more common. It is applied either to a fresh, not yet hardened sheet, or to a sheet after curing. The main enemy of painting is efflorescence: the lime of the cement comes to the surface and with carbon dioxide from the air gives white stains. This happens first of all during curing. So a coating on a fresh sheet can act at once as a barrier against efflorescence, while when a hardened sheet is painted, efflorescence and dust must be removed before the paint, otherwise they end up under the film. For a cement sheet, paints designed for an alkaline mineral substrate are used: most often water-based acrylic dispersions, less often silicate compositions. The requirements for a painted sheet (colour to the reference, evenness without stains and efflorescence, abrasion resistance of the coating) are set by GOST 30340-2012 for corrugated and GOST 18124-2012 for flat sheets.
What the owner and the process engineer need to decide
- At what stage to paint. This decides where to put the painting section: right after forming and before the chamber, or after curing before packing. Drying, stacking and rejects depend on it.
- Which paint to use. It is decided together with the paint supplier: which substrate (fresh or hardened sheet), application method, drying, resistance to sticking in the stack. Before buying a batch, make a trial coat on your own sheets.
- How to check. Colour references, a log of coating thickness and consumption, an abrasion test to GOST. Without a reference, a dispute with the buyer over colour cannot be settled.
Fresh sheet or hardened
| On a fresh sheet | On a hardened sheet | |
|---|---|---|
| Efflorescence | the coating covers the surface while the lime is only coming out | efflorescence may already have come out, so it is removed before painting |
| Adhesion | the paint enters a still open surface; a paint designed for a damp substrate is needed | the substrate is dry and strong; a clean, dust-free surface is needed |
| Drying | the sheet goes on to the chamber, and the coating dries together with curing | separate drying is needed, often with heating |
| Risk | damaging the soft sheet during application, sticking to the spacers | efflorescence under the film, dust, peeling |
| Stack | the sheets are still wet and warm, so there is a risk of sticking | the sheets are warm after drying, so there is also a risk of sticking |
A patent from one of the makers of coating binders states directly that lime efflorescence appears as the cement sets, so it is sensible to apply the coating before hardening, on a fresh sheet; but it also discusses an option for protecting an already hardened sheet.
Which paints
- Acrylic water-based dispersions. The most common option for fibre-cement sheets: binder manufacturers make acrylic emulsions specifically for cement facade and roofing sheets, including corrugated ones. They form a water-repelling film on the surface.
- Silicate (mineral) paints. They do not form a separate film but bond chemically with the mineral substrate. They suit mineral surfaces; their applicability to a particular sheet is confirmed from the manufacturer's technical data sheet.
- Colouring in the mass. Pigment is added to the slurry and the colour runs through the whole thickness of the sheet. Efflorescence on the surface is still possible, so such a sheet may also be covered with a protective composition.
Where painting defects come from
| What is seen | Where the cause is |
|---|---|
| White stains under the paint or over it | efflorescence: paint applied to a sheet with lime still coming out, too thin a layer, the sheet got wet in the stack |
| Stains and colour variation | uneven layer: nozzles, pressure, conveyor speed; different absorbency of the sheet |
| Peeling | dust, efflorescence or oil from the spacers on the surface; paint not meant for an alkaline substrate |
| Sheets stuck together in the pack | coating not fully dry or soft, sheets stacked warm; no anti-sticking layer on the back |
| Paint wears off on the crests | thin layer, under-drying; checked by the abrasion test to GOST |
What is checked to GOST
GOST 30340-2012 and GOST 18124-2012 require of a painted sheet: colour and intensity to an approved reference or catalogue; even colouring, without efflorescence and stains visible from a set distance; a coating that withstands the abrasion test with quartz sand. These standards set no requirements for the adhesion of the coating: it is checked by the paint supplier's method. What applies in your country is checked in the national register of standards.
How we do it
- From a number, drawing or photo of the unit, we look for the item at the manufacturing plant. What we find, with the price, photos and specifications, we send before the order.
- We check the batch at the plant before shipment: article number, dimensions, batch, packaging.
What this article relies on
Below are the documents and materials we refer to, so that you can check what is said for yourself.
Standards and documents
- GOST 30340-2012 "Corrugated chrysotile-cement sheets. Specifications" (Листы хризотилцементные волнистые. Технические условия): requirements for painted sheets: colour to the reference, evenness, efflorescence and stains, abrasion with quartz sandtext ↗
- GOST 18124-2012 "Flat chrysotile-cement sheets. Specifications" (Листы хризотилцементные плоские. Технические условия): the same requirements for painted flat sheetstext ↗
Reference materials
- Patent US 8754151 "Multistage polymer dispersions, processes for preparing them, and use thereof": the cause of efflorescence on fibre cement, coating of a fresh and a hardened sheet, application methods, sticking of painted sheets in a warm stackpatents.google.com ↗
- Dow, PRIMAL ICC-4: an acrylic emulsion for coating cement facade and roofing sheets, including corrugated onesdow.com ↗
- Caparol, DisboROOF 412: an acrylic roof coating for fibre-cement sheets (repainting on site)caparol.de ↗
- "Silicate mineral paint" (Wikipedia): silicate paint bonds with the mineral substrate and is poorly suited to non-mineral onesen.wikipedia.org ↗
- "Technology of Production of Building Materials, Products and Structures" (Технология производства строительных материалов, изделий и конструкций) (bibliotekar.ru): coloured asbestos-cement products: dyes, coloured varnishes, enamels and resinsbibliotekar.ru ↗
- Environmental declaration for corrugated fibre-cement sheets (heinze.de): painted sheets, anti-sticking treatment of the backheinze.de ↗
The comparison "on a fresh sheet versus a hardened one" and the defect table are conclusions from the sources named; no plant regulations for painting slate were found in open access. Coating thickness, drying and settings for your line are set by the regulations and the paint's technical data sheet.