0In the list
02Defects and testing

How a lot of slate is accepted: sampling and retesting

A lot of slate is the shift output of one line. Every lot goes through acceptance tests: appearance, dimensions, load or bending, density. The other indicators are checked periodically. Sheets for checking are taken from different stacks, leaving out the outer ones. If the defects fall between the acceptance number and the rejection number, a second sample is taken. If a periodic test fails, control is switched to every lot.

Updated 4 min read

In short

4minutes to read

7sections

3sources

3catalog items

In this article

  1. 01What the owner and the head of OTK need to decide
  2. 02Two kinds of tests
  3. 03How sheets are selected
  4. 04If the result is borderline
  5. 05If a periodic test fails
TableTwo kinds of tests5 rows →
Contents
  1. What the owner and the head of OTK need to decide
  2. Two kinds of tests
  3. How sheets are selected
  4. If the result is borderline
  5. If a periodic test fails
  6. Acceptance at the buyer
  7. How we do it

A lot of slate is accepted by rules that since 2013 have been in the sheet standards themselves: GOST 30340-2012 for corrugated and GOST 18124-2012 for flat. Before that they were in GOST 30301-95. A lot is sheets of one type, made by one process from the same materials in one shift on one line. Every lot goes through acceptance tests. The other indicators are checked periodically, on one lot a month or a quarter. Sheets for checking are selected from different stacks, and the outer sheets are not taken. The decision to accept or reject depends on the number of defective sheets in the sample. If the result is borderline, a second sample is taken and the defects are counted together.

What the owner and the head of OTK need to decide

  • Do not blur the lot. A lot is one shift of one line. If the log has a lot "for a day" or "for a week", then in a claim the good sheets cannot be separated from the bad, and everything falls under suspicion.
  • Do not pick good sheets for checking. The standard directly forbids selecting the best or the worst. A handsome report on selected sheets will not protect the plant from a buyer's claim.
  • Know what happens after a failure. Failing a periodic test switches the line to checking every lot. That is a load on the laboratory, and it has to be planned for.

Two kinds of tests

Acceptance tests: on every lot

Corrugated sheet (GOST 30340)Flat sheet (GOST 18124)
appearanceappearance
dimensions and shapedimensions and shape
punch or bar loadbending strength
densitydensity
resistance of the colored coatingresistance of the colored coating

Periodic tests: on one lot from the line

  • Corrugated sheet: bending strength and impact toughness at least once a month; frost resistance and water tightness at least once a quarter.
  • Flat sheet: impact toughness about once a month, frost resistance once a quarter.

How sheets are selected

  1. Sheets are taken from different stacks, no more than one sheet from a stack.
  2. The two top and two bottom sheets of a stack do not go into the sample.
  3. Selection is random, without picking the best and the worst.
  4. For routine acceptance the manufacturer takes three sheets. If an indicator fails, and also when the buyer checks the lot, sampling inspection is used: the sample size grows with the size of the lot, and the standard sets it in a table together with the acceptance number and the rejection number: how many defective sheets are allowed and at how many the lot is rejected.
  5. The selected sheets and the specimens cut from them are marked, so that the result can later be tied to the lot.

Appearance and dimensions are checked on the whole sample. For physical and mechanical tests, several sheets are taken from it and specimens are cut.

If the result is borderline

If the number of defective sheets is greater than the acceptance number but less than the rejection number, no decision is made on the first sample. A second sample of the same size is taken, checked, and the defects of the two samples are added up. The total is compared with the numbers for the combined sample. This is how the standard guards against error in both directions: a good lot is not rejected because of one unlucky sheet, and a bad one is not accepted because of a lucky sample.

If a periodic test fails

If a periodic test gives an unsatisfactory result, control of that indicator is switched to every lot. The line returns to periodic control after ten lots in a row have shown a positive result. For a corrugated sheet, GOST 30340 makes an exception for frost resistance. A flat sheet under GOST 18124 is switched to control of every lot if it fails on impact toughness.

In parallel the process engineer looks for the cause. A failure in bending or impact is almost always tied to the mass, the felt, the press or curing: see the articles on cracks, delamination and a brittle sheet.

Acceptance at the buyer

The buyer has the right to check the lot by the same rules and methods. That is why the test logs, the lot marking and the quality document must agree with one another. The standard directly calls the test logs an official document of the manufacturer.

How we do it

  • From the photo, dimensions and the passport of the unit, we look for the item at the manufacturing plant. What we find, with the price, photos and specifications, we send before the order.
  • We inspect the lot at the plant before shipment: part number, dimensions, lot, packaging.

What this article relies on

Below are the documents and materials we refer to, so that you can check what is said for yourself.

Standards and documents

  • GOST 30340-2012 "Chrysotile-cement corrugated sheets. Specifications", the section "Acceptance rules": lot, acceptance and periodic tests, selection, second sample, switch to control of every lot; replaced GOST 30301-95 as far as corrugated sheets are concernedtext ↗
  • GOST 18124-2012 "Chrysotile-cement flat sheets. Specifications", the section "Acceptance rules"text ↗
  • Record card of GOST 18124-2012 on meganorm.ru: what it replaces (GOST 18124-95, parts of GOST 8747-88 and GOST 30301-95)text ↗

Sample sizes, acceptance numbers and rejection numbers are in the tables of the standards; this is a retelling without figures.

Related catalog items

  • 001Three-station pneumatic stacker

    Three-station pneumatic stacker

    TMN-XHB-05Xinhuibo

  • 002Fiber-cement and asbestos-cement sheet production line

    Fiber-cement and asbestos-cement sheet production line

    TMN-XHB-01Xinhuibo

  • 003Hydraulic press 3000–15000 t

    Hydraulic press 3000–15000 t

    TMN-XHB-02Xinhuibo

For slate plants

Felts, meshes and units for your line

We select from manufacturing plants in China by nameplate photo and machine dimensions. Send a photo of the plate and we will tell you what can be ordered.

Request

Ask about your machine

A part number is enough. A drawing or a photo of the unit speeds up sourcing but is not required.

Up to 3 files: photos (JPG, PNG, WEBP, HEIC) or PDF, up to 15 MB in total