Flocculant in slate slurry: what it is for and how to choose one
A flocculant is a water-soluble polymer, usually anionic polyacrylamide. It gathers fine cement and silica into flocs, so that they stay on the screen and settle faster in the recuperator. It works in a small dose, and an overdose does harm: it shifts the setting times, hinders the release of water and can cause foam. The grade is chosen by a trial on your own machine, not from a catalog.
In short
10minutes to read
10sections
3sources
In this article
- 01What the technologist and the chief mechanic should decide
- 02Why it is the anionic flocculant that works
- 03How much to add and what an overdose does
- 04Where the flocs get broken
- 05Flocculant in the recycled water
Contents
- What the technologist and the chief mechanic should decide
- Why it is the anionic flocculant that works
- How much to add and what an overdose does
- Where the flocs get broken
- Flocculant in the recycled water
- How the solution is made up
- How to choose a grade
- Safety
- What to send if you need a flocculant or a makeup unit
- How we do it
A very thin slurry arrives at the screen of the cylinder: it holds fiber, cement, in fiber cement also ground quartz sand, and a lot of water. The openings of the screen are larger than the finest particles, so part of the cement and silica passes through the mesh together with the water. They cannot be lost: cement and silica are chemically active, and they have to be returned to the slurry quickly, before they lose their properties. For this a flocculant is added to the slurry and to the recycled water. It is a water-soluble polymer with a long molecule. It latches onto several particles at once and binds them into flocs. The flocs are larger, they stay on the screen and settle faster in the recuperator.
What the technologist and the chief mechanic should decide
- Which flocculant. For cement slurries anionic flocculants work. Most often this is a copolymer of acrylamide and acrylic acid, that is, anionic polyacrylamide.
- Where to add it. Into the mixing box before the vats and, if needed, also into the recycled water before clarification.
- How much. The dose is small, and it is chosen by a trial on the machine. An overdose harms the sheet and the machine.
- How to hold the quality. Lots of the same product can behave differently. A new lot is checked before it is put into work.
Why it is the anionic flocculant that works
The recycled water of a slate machine holds dissolved alkali and a lot of calcium from the cement. The authors of a study on choosing flocculants for a Hatschek machine, carried out at a working plant, explain it this way: in such water the particles of cement, silica and cellulose take a positive charge, so a flocculant with a negative charge, that is, an anionic one, sticks to them firmly. In practice it is precisely anionic flocculants that prove effective for cement slurries.
A flocculant has two main characteristics, and the supplier usually names only these:
| Characteristic | What it means | What it gives |
|---|---|---|
| Ionic charge, % | the share of acrylic acid units in the polymer | in laboratory tests with a fiber-cement slurry, the higher the charge, the faster the settling |
| Molecular mass | length of the molecule, in millions | a long molecule reaches several particles at once and binds them; on the Hatschek machine, flocculants with a mass of about 10–27 million worked better |
Two grades with the same figures in the passport can work differently. The authors of the same study link this to the spread of molecule length within a lot and to the branching of the chains. Suppliers usually do not disclose these data. At the same plant the "good" and the "bad" lots of one grade differed in molecular mass, and a difference in performance was found even between bags of one lot.
How much to add and what an overdose does
The dose of flocculant is measured in grams per tonne of solids or in fractions of a percent of the cement mass. On the machine in that study, the flocculant was fed as a 0.1% solution into the mixing box. The dose was varied from about 60 to 300 g per tonne of solids in the vat. This is the experience of one machine, not a norm: the dose depends on the cement, the fillers, the fiber and the water.
The laboratory study gave these results. Settling, water release and strength were studied on a fiber-cement slurry with cellulose and ground quartz sand, and setting and hydration on cement paste without fiber:
| Polyacrylamide addition, % of cement mass | What was observed |
|---|---|
| 0.05 | with the strongest grade (anionic, high charge) the settling of particles sped up 8 times |
| 0.05–0.15 | in cement paste the start of setting moved later and the end earlier than without the addition, by tens of minutes |
| 0.05–0.1 | with the anionic grade of high charge, the bending strength was 10–15% higher |
| over 0.1 (0.15 in the tests) | cement hydration weakens; the slurry holds water and gives it up worse during pressing |
Hence the rule: add exactly as much flocculant as is needed for retention and clarification, and no more. An overdose may show up as foam in the vats, and in laboratory tests, with an addition above 0.1%, the slurry gave up water worse during pressing. More flocculant does not mean better flocculation: in the study on the Hatschek machine, foam and even a complete absence of flocculation are directly named as a possible result of overdosing and incorrect use.
Where the flocs get broken
The flocs are held by weak bonds. Strong mixing and impact break them, and sometimes tear the flocculant molecules themselves. After that the flocculant works much worse, even if the mixing is later reduced.
At the plant in the same study, the slurry went from the mixing box to the vats through a centrifugal pump. The pump broke the flocs. The mixing box was raised and the slurry was sent to the vats by gravity, and the flocculant began to be added in the box downstream of the slurry feed. After that the share of solids retained on the screen rose from about 30% to 40–53%, and the foam almost disappeared. The time in the mixing box was enough for the flocculant to take effect.
What to check at your plant:
- whether there is a centrifugal pump between the point where the flocculant is added and the vat;
- whether there is enough time between the addition and the vat for the flocs to form.
Flocculant in the recycled water
Solids go into the recycled water with any flocculant. So an additional flocculant is usually added to the recycled water as well, after the pump, so that the solids settle faster in the settling tanks. The authors of the study allow that different grades may be needed for retention on the screen and for clarifying the water, but they did not check this systematically. How the closed water loop is arranged and what builds up in it is described in the article on recycled water.
How the solution is made up
- The powder is dissolved in drinking water in advance and fed to the machine as a solution. The working concentration is kept low: in both studies it is 0.1%, otherwise the solution is too viscous.
- Not every grade dissolves properly. At that plant several grades could not be dissolved to 0.1% at an acceptable viscosity, and they were dropped from the trials.
- The dissolving time, the makeup equipment and the shelf life of the solution are taken from the technical data sheet of the particular grade.
- The powder is stored in a dry place in a closed container, away from alkalis and oxidizers. The safety data sheet we read says the product is incompatible with strong bases and oxidizers, and that ammonia is released on contact with strong bases.
How to choose a grade
Laboratory tests are useful, but they do not predict the work on the machine. The authors checked several selection methods and concluded that the most reliable are short trials on the machine itself. The order is this:
- Stabilize the machine at a constant slurry concentration.
- Switch the flocculant off and wait until its effect disappears.
- Add the flocculant in steps, letting the machine stabilize at each step.
- At each step take samples of the slurry from the mixing box and the vat: filtrate volume per minute, solids in the filtrate, retention on the screen.
- Look at the sheet: moisture, density, formability. Some grades change these properties. At the plant in that study, the moisture of the wrap for corrugated sheet had to be adjusted for each grade, otherwise cracks appeared during corrugating.
A flocculant that works well with one cement and one recipe may work differently with others. If you change the cement or the fiber, repeat the trial. The studies we rely on were made on fiber-cement slurries. For asbestos-cement slurry too, the grade and the dose are chosen by a trial on your own machine.
Safety
The anionic flocculant whose safety data sheet we read is not classified as hazardous under the CLP regulation (EC) No. 1272/2008. The main hazard is different: wet powder and solutions make the floor extremely slippery. Hence the rules from the same data sheet:
- do not wash spilled powder away with water, but sweep it up or collect it with a vacuum cleaner; wash off the remains only after the cleanup;
- work in safety glasses with side protection and in gloves of PVC or another plastic; the powder can irritate the skin in folds and under tight clothing and moderately irritate the eyes;
- if it gets into the eyes, rinse at once with plenty of water for at least 15 minutes, and see a doctor if the irritation persists;
- when dust is raised, local exhaust is needed, and if there is more than 10 mg/m³ of dust in the air, a dust mask;
- rinse the empty container with water and use this water to make up the working solution.
Every grade has its own safety data sheet. Before work, read the data sheet of the grade that has arrived at the plant.
What to send if you need a flocculant or a makeup unit
- The grade you use now and its data sheet or technical data sheet: charge, molecular mass, supply form (powder or emulsion).
- Where you add the flocculant, at what concentration and with what dose.
- What is wrong: loss of solids, foam, turbid water in the settling tanks, wet wrap, cracks during corrugating.
- The type of product: asbestos cement or fiber cement, the fiber, the cement.
- The scheme of feeding the slurry from the mixing box to the vats: by pump or by gravity.
How we do it
- From the grade, the data sheet and the description of the task, we look for a product with the same characteristics at the manufacturing plant. What we find, with the safety data sheet and the technical data sheet, we send before the order.
- We work under a contract with the manufacturing plant. We inspect the lot at the plant before shipment: grade, lot, marking, packaging.
- Defects confirmed by a report are replaced: the replacement is supplied by the manufacturing plant under the contract.
What this article relies on
Below are the documents and materials we refer to, so that you can check what is said for yourself.
Reference materials
- Mukhametrakhimov R. Kh. "Cement-fiber compositions modified with flocculating additives" (Цементно-волокнистые композиции модифицированные флоккулирующими добавками) // Construction of Unique Buildings and Structures. 2018. No. 10(73). Pp. 28–37. DOI 10.18720/CUBS.73.3: purpose of flocculants, charge and molecular mass of polyacrylamide, 0.1% working solution, effect of 0.05–0.15% on setting, hydration, water release and strengthunistroy.spbstu.ru ↗
- Cooke A. M., Akers S. A. S., Leite J. V., Winter R. "Selection and performance of flocculants for Hatschek made air cured fibre cement", IIBCC 2010: anionic flocculants for cement slurries, molecular mass 10–27 million, spread between lots, dosing as a 0.1% solution into the mixing box (60–300 g/t), breaking of flocs by the pump, foam on overdose, selection by trials on the machineiibcc.biz ↗
- SNF, safety data sheet FLOPAM AN 923 SEP (anionic flocculant), revision of 27.01.2023: classification, slipperiness of the wet product, cleanup of spills, first aid, protective equipment, storage and incompatibility, rinsing of containersconsult.environment-agency.gov.uk ↗
The figures for doses and effects are taken from tests on particular slurries and machines and are not a norm. The grade and the dose for your line are chosen by a trial on the machine, following the process regulations of the plant.